SterlingStar Silver-III matte silver process is engineered specifically for electronic packaging and surface treatment. It is highly suited for silver plating on LEDs and communication components, and is fully compatible with rack plating, barrel plating, and high-speed reel-to-reel electroplating equipment. This process delivers a matte silver coating across a wide current density range, offering high current deposition efficiency, a highly stable process, and ease of control.
1. Process Features
(1) Applied in electronic packaging and communication component surface treatment technologies; suitable for rack plating, barrel plating, and high-speed reel-to-reel electroplating.
(2) A highly stable process with easy operation and high current deposition efficiency.
(3) The resulting silver deposit exhibits excellent electrical conductivity and solderability.
(4) The coating is organic-free (contains no organic matter).
(5) Silver purity is 99.99%.
2. Equipment Requirements
Plating Tank / Vessel:Steel tank with hard rubber lining, or plastic tank with plastic lining.
Anode:Pure silver anodes (silver purity > 99.9%).
Heating:Electric heaters or heating via heat exchangers.
Filtration:Continuous filtration.
Agitation:Cathode movement (rocking) agitation or high-speed agitation.
Rectifier:Maximum ripple must not exceed 5%.
3. Process Conditions
Rack and Barrel Plating Operations
| Parameters | Optimum | Range |
| Silver Metal | 25 g/L | 10–30 g/L |
| Free Potassium Cyanide | 50 g/L | 40–120 g/L |
| SterlingStar Silver-III MU (Make-Up) | 50 ml/L | 50 ml/L |
| SterlingStar Silver-III REP (Replenisher) | 15 ml/L | 10–20 ml/L |
| Bath Temperature | 30°C | 25–35°C |
| Cathode Current Density | 0.5 A/dm² | 0.2–1.5 A/dm² |
High-Speed Plating Operations
| Parameters | Optimum | Range |
| Silver Metal | 45 g/L | 41–49 g/L |
| Free Potassium Cyanide | 60 g/L | 50–70 g/L |
| SterlingStar Silver-III MU (Make-Up) | 50 ml/L | 50 ml/L |
| SterlingStar Silver-III REP (Replenisher) | 15 ml/L | 10–20 ml/L |
| Temperature | 50°C | 40–60°C |
| Current Density | 20 A/dm² | 15–25 A/dm² |
| Plating Efficiency | 25 μm/min at 40 A/dm²,equivalent to 4 g/Ah | |
| Agitation Method | Jet agitation or high-speed agitation | |
4. Bath Maintenance
(1) Silver Metal
Perform regular chemical analysis to guide replenishment, keeping the silver content of the plating bath within the specified process limits.
(2) Free Potassium Cyanide
It is recommended to maintain the free potassium cyanide concentration in the plating bath above 40 g/L. Ensure regular analysis and replenishment are performed.
• If below 40 g/L: The deposit may become hazy, and burning may occur in high current density (HCD) areas.
• If above 60 g/L: Low current density (LCD) areas may become bright (which may affect the desired matte finish).
| Product Name | Function | Consumption Rate |
| SterlingStar Silver-III MU | Matte Silver Make-up; contains the primary brightener. | Used only during bath make-up (initial setup). |
| SterlingStar Silver-III REP | Matte Silver Replenisher; contains the auxiliary brightener. | 100–150 ml/KAH |
5. Deposition Rate
| Current Density (A/dm²) | 10 | 20 | 30 | 40 |
| Coating Thickness (inch) | Required Time (minutes) | |||
| 0.0001 | 3.75 | 1.8 | 1.3 | 0.9 |
| 0.0002 | 7.50 | 3.6 | 2.6 | 1.8 |
| 0.0003 | 11.25 | 5.4 | 3.9 | 2.7 |
| 0.0004 | 15.00 | 7.2 | 5.2 | 3.6 |
| 0.0005 | 18.75 | 9.0 | 6.5 | 4.5 |
| 0.0006 | 22.50 | 10.8 | 7.8 | 5.4 |
| 0.0007 | 26.25 | 12.6 | 9.1 | 6.3 |
| 0.0008 | 30.00 | 14.4 | 10.1 | 7.2 |
| 0.0009 | 33.75 | 16.2 | 11.7 | 8.1 |
| 0.0010 | 37.50 | 18.0 | 13.0 | 9.0 |
6. Analytical Methods
6.1 Silver Content
1. Pipette 2 ml of the plating solution into a 300 ml Erlenmeyer flask.
2. In a fume hood, accurately add 10 ml of concentrated sulfuric acid (H₂SO₄) and 10 ml of concentrated nitric acid (HNO₃).
3. Boil the solution until the precipitated silver sulfide (Ag₂S) is completely dissolved.
4. Cool the flask, then carefully add 100 ml of distilled water and approximately 2 ml of ferric ammonium sulfate indicator solution (20 g/L).
5. Allow the solution to cool completely.
6. Titrate with 0.1 N potassium thiocyanate (KSCN) solution until a persistent reddish-brown end point is reached.
Calculations:
• A x 5.4 = g/L Silver (Ag)
• A x 6.7 = g/L Potassium Cyanide (KCN)
• A x 10 = g/L Potassium Silver Cyanide [KAg(CN)₂]
(Where A = ml of 0.1 N KSCN titrant used)
6.2 Free Cyanide
1. Pipette 2 ml of the plating solution into a 300 ml Erlenmeyer flask.
2. Add 100 ml of distilled water and approximately 5 ml of potassium iodide (KI) indicator solution (100 g/L).
3. Titrate with 0.1 N silver nitrate (AgNO₃) solution until a faint, permanent turbidity (cloudiness) is reached as the end point.
Calculation:
A x 6.5 = g/L Free Potassium Cyanide (KCN)
(Where A = ml of 0.1 N AgNO₃ titrant used)
7. Product Information
7.1 SterlingStar Silver-III MU (Matte Silver Make-up)
• Appearance: Colorless, transparent liquid
• pH Value: 10.8–13.2
• Specific Gravity: 0.998–1.012
7.2 SterlingStar Silver-III REP (Matte Silver Replenisher)
• Appearance: Colorless, transparent liquid
• pH Value: 9.5–11.0
• Specific Gravity: 0.995–1.005
8. Silver Strike Process
| Parameters | Specification / Range |
| Silver Metal | 1–2 g/L |
| Potassium Cyanide | 70–90 g/L |
| Temperature | Room temperature (RT) |
| Current Density | 1–2 A/dm² |
| Anode Material | Stainless steel plate |
| Plating Time | 5–10 seconds |
9. Environmental Protection
The silver plating solution contains cyanide. Both the solution and its rinse water must be properly treated prior to discharge in compliance with national and local regulations.
10. Product Warranty
We stand behind the quality of our products. However, this warranty does not cover damages or failures caused by improper handling or incorrect usage by the customer. Our technical support team is always available to assist with any questions or troubleshooting required during use.
11. Disclaimer
The information, suggestions, and recommendations concerning our products in this instruction manual are based upon laboratory testing and data believed to be reliable. Since the actual conditions of use and handling by third parties are beyond our control, we make no guarantee of results and assume no liability for any damages or adverse consequences. Nothing contained herein is to be construed as a recommendation to use any product in conflict with any existing patents or copyrights.