TinStar HM-411-1 is suitable for high-speed plating, barrel plating, and rack plating. It is a strongly acidic, fluoride-free pure tin plating electrolyte. It produces fine-grained, silk-matte deposits. The tin is deposited with a crystalline structure having a grain size of 3–8 µm. Compared to bright tin deposits with grain sizes under 1 µm, it exhibits an extremely low tendency for whisker formation. After thermal aging at 155°C for 16 hours, the coating still maintains excellent solderability. Developed as a lead-free electroplating process for various types of components, the deposit is highly compatible with lead-free tin-based solder alloys, featuring fast wetting speed and excellent low-current-density coverage (throwing power).
Plating Tank: Rubber-lined steel plate, PVC (polyvinyl chloride), or PP (polypropylene).
Circulation: 6–8 bath volumes per hour.
Filtration: Continuous filtration is recommended.
Anode: Pure tin anodes (99.95%) conforming to DIN 1704 (Germany) / BS ED161 (UK).
Heating: Immersion ceramic heaters.
| Specific Gravity | Dosage | |
| Methanesulfonic Acid (MSA) | 1.33 | 8 L |
| Tin Methanesulfonate (MST) | 1.53 | 22 L |
| TinStar HM-411-1 (Matte Tin Additive) | 1.03 | 4 L |
| Parameter | Range | Optimum Value |
| Stannous Tin (Sn2+) | 60–80 g/L | 70 g/L |
| Methanesulfonic Acid (MSA) | 70–90 ml/L | 80 ml/L |
| TinStar HM-411-1 (Matte Tin Additive) | 30–50 ml/L | 40 ml/L |
| Temperature Range | 40–50 °C | 45 °C |
| Cathode Current Density | 10–80 A/dm² | 10–80 A/dm² |
| Anode Current Density | < 60 A/dm² | < 60 A/dm² |
| Deposition Rate (at 20 A/dm²) | 10 μm/min | 10 μm/min |
Bath Makeup Procedure (for 100 Liters)
Add Deionized Water: Fill the plating tank with 60 L of deionized (DI) water.
Add Methanesulfonic Acid (MSA): Carefully add 8 L of methanesulfonic acid (MSA) and mix thoroughly.
Add Tin Methanesulfonate (MST): Carefully add 22 L of tin methanesulfonate (MST) and mix until completely uniform.
Add Additive: Add 4 L of TinStar HM-411-1 (Matte Tin Additive) and mix well.
Final Dilution & Mixing: Add the remaining DI water to reach the final volume, stir thoroughly to ensure homogeneity, and the solution is ready for test plating.
| Parameter | Range | Optimum Value |
| Stannous Tin (Sn2+) | 30–40 g/L | 36 g/L |
| Methanesulfonic Acid (MSA) | 80–120 ml/L | 100 ml/L |
| TinStar HM-411-1 (Matte Tin Additive) | 30–50 ml/L | 40 ml/L |
| Temperature Range | 30–50 °C | 40 °C |
| Cathode Current Density | 0.5–2 A/dm² | 1.5 A/dm² |
| Anode Current Density | Not critical | Not critical |
| Deposition Rate (at 1.5 A/dm²) | 0.75 μm/min | 0.75 μm/min |
Bath Makeup Procedure (for 100 Liters)
Add Deionized Water: Fill the plating tank with 70 L of deionized (DI) water.
Add Methanesulfonic Acid (MSA): Carefully add 10 L of methanesulfonic acid (MSA) and mix thoroughly.
Add Tin Methanesulfonate (MST): Carefully add 12 L of tin methanesulfonate (MST) under continuous stirring, and mix until completely uniform.
Add Additive: Add 4 L of TinStar HM-411-1 (Matte Tin Additive) and mix well.
Final Dilution & Mixing: Add the remaining DI water to reach the final volume, stir thoroughly to ensure homogeneity, and the solution is ready for test plating.
Notes:
1. Consumption & Replenishment
The consumption of the additive is mainly due to drag-out losses, which depend on the tank design and workpiece geometry.
2. Deposit Properties
The deposit contains a very low carbon content from the additive, at only 0.003%. Even after standard aging tests, the deposit retains excellent solderability and can be reflowed in an electric furnace or oven.
3. Pretreatment
Conventional pretreatment is required. Our company provides a complete range of pretreatment processes.
Tin (Sn)
The cathode current efficiency of the tin bath is approximately 97%. Even at high current densities, replenishment of tin salts is rarely required, as drag-out losses are compensated for by anode dissolution. However, if tin supplementation is necessary, it can be replenished using Tin Methanesulfonate (MST).
Methanesulfonic Acid (MSA)
Replenish the acid concentrate based on analytical titration results.
TinStar HM-411-1 (Matte Tin Additive)
The additive content can be determined by analysis and adjusted accordingly. If chemical analysis is not feasible, it can be replenished based on production throughput at 2–5 mL/m² or 0.4 kg/kAh. Accidental overdosing has no adverse effect on the process.
An insufficient concentration of TinStar HM-411-1 additive will lead to reduced coverage (throwing power) in low-current-density areas. This can be corrected by dosing in increments of 5–10 mL/L. The additive is non-foaming, even under vigorous solution agitation.
Troubleshooting Guide
| Issue / Defect | Probable Cause | Corrective Action |
| Poor coverage (throwing power) in low-current-density areas | Insufficient TinStar HM-411-1 | Add 5–10 mL/L of additive |
Wastewater Treatment
The plating solution contains no complexing agents. Rinse water should be neutralized to pH 7–9 using sodium hydroxide (NaOH).
Health & Safety
The plating solution contains methanesulfonic acid and is corrosive. When handling the bath or raw chemical materials, protective clothing, chemical-resistant gloves, and safety goggles must be worn.
In case of contact with skin or eyes, flush immediately with plenty of running water for 10–15 minutes. If irritation, pain, or inflammation persists, seek medical attention immediately.
All recommendations and suggestions regarding our company's products in this manual are based on experiments and data we deem reliable. Since we cannot control the actual operations of other practitioners, our company cannot guarantee or be held responsible for any adverse consequences.