PalladiStar PN-2900

Column:Palladium Plating Additive

1. Introduction

PalladiStar PN-2900 is a high speed palladium-nickel process that is specially designed to deposit palladium-nickel alloys (80/20) for electronic components. The resulting deposit has a nominal 80 wt% Pd, but may be modified to produce 70 – 90% Pd. The deposits are stable with less than ± 5% variation over the current density range of 10 – 120 ASD. Deposits are also bright and ductile which are required for excellent contact stability. In addition, palladium-nickel alloys exhibit lower porosity and better wear resistance than either hard gold or pure palladium. This makes PalladiStar PN-2900 a great choice for highly reliable connector systems. This solution yields a very high plating rate and is easy to maintain using standard techniques. The PalladiStar PN-2900 process operates at neutral pH and is less corrosive than other conventional processes. The PalladiStar PN-2900 process uses less ammonia and is virtually odorless.

2. Characteristics

  • Halogen free

  • Good corrosion resistance

  • High wear resistance

  • Low porosity

  • Less ammonia odor

3. Deposit Characteristics

  • Hardness: 450 to 650 mHV10

  • Current Density: 10 – 120 ASD

  • Composition: 80% (wt) Pd ± 10% (rest is nickel)

  • Deposit Density: 10.7 g/cm3

  • Weight: 2.7 mg/cm2 for 2.5 micron

  • Contact Resistance: < 4 mΩ

4. Materials

  • Palladium Salt No 2

  • PalladiStar PN-2900 MU

  • PalladiStar PN-2900 ADD A

  • PalladiStar PN-2900 ADD B

  • PalladiStar PN-2900 NI

  • PalladiStar PN-2900 Conducting Salt

  • Boric Acid

  • sulfuric Acid 96%

  • Ammonium Hydroxide 28% (NH4OH)

Palladium Salt No 2
It is a salt and contains about 38.5% palladium metal, required for make-up and replenishment.

PalladiStar PN-2900 MU
Contains nickel and additives, required for make-up of the operating solution (without palladium).

PalladiStar PN-2900 ADD A
For replenishment of stress reducers.

PalladiStar PN-2900 ADD B
Contain the additives, required for replenishment of wetter and pH buffer.

PalladiStar PN-2900 NI
For replenishment of Nickel.

PalladiStar PN-2900 Conducting Salt
Is required to provide bath conductivity.

Boric Acid
Is required to maintain pH.

Ammonium Hydroxide (NH4OH) reagent grade
Is used to raise the pH.

5. Equipment

Tank
Use Pyrex, polytetrafluoroethylene (PTFE), natural (unfilled) polypropylene, PVC or high-density polyethylene supported externally.

Rectifier
A standard DC power supply, with less than 5 % ripple and with an ampere output capacity sufficient to meet the requirements of the plating operation is required. The unit should be equipped with a voltmeter, an ammeter, and stepless control for accurate regulation of the current. Use of an ampere minute meter is strongly recommended.

Anodes
Anodes of platinized titanium or niobium, platinum clad titanium or niobium or pure platinum. Platinized titanium with an area sufficient to provide a maximum anode current density of 0.3 ADS is recommended.

Filtration
The solution must be filtered continuously preferably through a 1 micron (and at least 5 microns) polypropylene cartridges to maintain clarity. Before using, soak the cartridges for several hours in 10% sodium hydroxide at 60 ºC (140 ºF), then rinse well in running water and finally, soak the cartridges in 50 % ammonium hydroxide solution.

Agitation
Moderate, mechanical agitation of the pieces together with the solution agitation by means of the filter pump help ensure uniformity of deposits and eliminate pitting on the plated articles.

Temperature Control
Immersion heaters such as porcelain, titanium or PTFE may be used. It is important to have adequate solution agitation around the heaters to avoid local hotspots. Heaters with a low heat density per unit area are the most suitable.

Ventilation
Exhausting system is recommended for high speed plating. Please take note of the local regulations.

6. Chemical Composition


OptimalRange
Palladium (g/l)1614 - 18
Nickel (g/l)2018 - 25
Density (g/cm3)1.10> 1.10
Boric Acid (g/l)1510 - 18
PalladiStar PN-2900 Conducting Salt (g/l)10070 - 130
pH7.27 - 7.35
Temperature (ºC)4540 - 55
Ratio of anode/cathode2:11:1 - 5:1
Cathode current densityDependent of electrolyte agitation (A/dm2)
10 - 120
Efficiency (mg/Amin)2624 - 28
Time to deposit 1 micron at 10 A/dm2 (sec.)3028 - 35

7. Initial Make-up of the Solution

The make-up solution is supplied as a liquid PalladiStar PN-2900 MU, it does not contain precious metal.

The following materials are required for the bath (100 liter):

  • PalladiStar PN-2900 MU: 60 liters

  • Palladium Salt No 2: 4156 grams

  • Boric Acid: 1500 grams

  1. The plating tank, filter pump, anodes and anode bags must be properly leached with a 10% v.v. sulfuric acid solution and thoroughly rinsed with water.

  2. The plating tank, filter pump, anodes and anode bags must be properly leached with a 10% v.v. ammonium hydroxide solution and thoroughly rinsed with water.

  3. Fill the tank with 25% of the required volume with deionized or distilled water.

  4. Fill the tank with required PalladiStar PN-2900 MU and heat up the solution to 45°C.

  5. Add, in a separate tank with warm PalladiStar PN-2900 MU, with agitation, the required quantity boric acid and stir until it has completely dissolved. Filtrate back in to working tank.

  6. Add, in plating tank, with agitation, the required quantity Palladium Salt No 2 and stir until it has completely dissolved.

  7. Adjust the final volume with deionized or distilled water.

  8. Adjust the pH of the bath to 7.2 electrometric with ammonium hydroxide 10% v.v. or sulfuric acid 10% v.v.

  9. Control and maintain temperature at 45°C.

  10. Keep circulation for at least 1 hour before use.

8. Process Optimization

The suggested solution composition above may not provide the optimum solution performance in every situation. The following set of guidelines is provided to assist in achieving ideal performance.

Palladium and Nickel Concentration
The metal concentration required to properly operate the solution is dependent on balancing the plating rate, agitation speed and minimizing drag-out losses. If the plated deposit shows the effects of "burning" (i.e. dark gray to black nodular or powdery deposits) due to excessive current density, then lower the current density or increase the Pd and Ni concentration and/or solution agitation. The ratio of Pd to Ni metal should generally be maintained to provide consistent deposit composition.

9. Process Control

Palladium and Nickel Replenishment and Control
The alloy composition in the deposit is directly related to Ni/Pd ratio in the operating solution within the specified range (10 to 30 % Ni) as pH, current density, temperature and agitation are held constant. Palladium and nickel concentrations in the operating solution should be maintained within 10 % of the desired values. However, it is recommended to replenish palladium and nickel after each 2 % depletion. The more frequently the metals are replenished, the more stable the bath performance. The concentration of Pd and Ni concentrations should be determined quantitatively once per day or as required.

Under standard conditions, the plated alloy contains 80 % Pd. For 125 g of plated alloy (100g Pd = 2600A/min) add:

  • Palladium Salt No 2: 260g

  • PalladiStar PN-2900 ADD A 250mL

  • PalladiStar PN-2900 ADD B 500mL

  • PalladiStar PN-2900 NI 250mL

Addition of PalladiStar PN-2900 NI (1ml/l) will increase 0.1g/l of Nickel.

pH Control
The pH should be within the range of 7.0 to 7.35 when measured at room temperature. It is advised to initially set the pH at 7.2 and maintain it within +/- 0.2 units. The pH should be measured at room temperature at least twice per shift using a calibrated pH meter. If the pH is low and needs to be raised, add NH4OH, mix and re-check. If the pH is high and needs to be lowered, add sulfuric acid 10%, mix and re-check.

Temperature Control
The temperature should be maintained in the range of 40 to 55 °C. The typical temperature is 45 °C.

10. Process Maintenance

This chemistry has demonstrated satisfactory long term performance without operating solution regeneration. However, performance can deteriorate whenever organic or metallic contaminants are introduced. The diagnostic Hull Cell is utilized to determine the presence of these contaminants. The procedures below can be used to regenerate a contaminated operating solution.

Carbon Treatment
After excluding the possibility of metallic contamination (Cu, Fe, Zn, etc.) through trace metal analysis, a carbon treatment should be applied. For detail information, please contact our technical service
Important: Don’t bring in cyanide in to the electrolyte.

Removal of Metallic Contaminants
Copper may accumulate in the operating solution when copper or copper alloy substrates are used. The build-up of copper should be minimized through "live" entry, i.e. immersion of substrates under applied voltage. The presence of copper may be confirmed by analysis (i.e. atomic absorption) and/or Hull Cell diagnostic. The copper content should be kept below 50 ppm by "dummying" whenever required. Dummy plating is performed with cathodes of the size of 0.1 to 0.2 ft2 per liter of solution at current densities of 0.02 to 0.05 ASD.

11. Waste Treatment

Do not dispose of untreated working solution. Waste must be disposed of in accordance with local environmental control regulations, it is user’s responsibility to verify that treatment and disposal procedures comply with local environmental control regulations.

12. Handling and Safety Precautions

Hazards
For detailed information consult the material safety data sheets for this product. Please read material safety data sheets carefully before using this product.

First Aid
In case of contact of PalladiStar PN-2900 or the operating solution with skin or eyes, flush with plenty of clean, cool water for 15 minutes. If eye irritation develops, get medical attention. Remove and wash contaminated clothing and shoes. Contact medical immediately if ingested or not feeling well due to prolonged inhalation.

Handling Information
When handling any chemicals used in the PalladiStar PN-2900 process, always wear proper personal protective equipment, i.e. protective clothing, safety goggles, face shield, respirator and gloves. In case of skin contact, immediately flush with clean water. In case of eye contact, immediately flush with clean water and obtain medical aid. Please refer to SDS for further handling and safety information.

Storage
Storage room should be dry and well ventilated.

13. Disclaimer

The information presented herein is to the best of our knowledge true and accurate and all recommendations and suggestions appearing in this document covering the use of our products are based upon information believed to be reliable. However, users should conduct their own tests or experiments to determine the suitability of these products for their own particular purposes, since the company will not be liable to any person in contract, tort (including negligence), liability for any claims, damages, losses whatever or risk involved in the use these products. No warranties, expressed or implied, are made regarding the information, product, processes, recommendations, description and safety notations contained herein. Nothing herein shall be deemed a recommendation to use any product or process in violation of any patent rights.